AISI 50B46 | |
Conditions | Tensile Properties | ||
T (°C) | Treatment | ||
25 | oil quenched, fine grained, tempered at 315°C | Tensile Strength (MPa) | 1779 |
Yield Strength (MPa) | 1620 | ||
Elongation (%) | 10 | ||
Reduction in Area (%) | 37 | ||
25 | oil quenched, fine grained, tempered at 425°C | Tensile Strength (MPa) | 1393 |
Yield Strength (MPa) | 1248 | ||
Elongation (%) | 13 | ||
Reduction in Area (%) | 47 | ||
25 | oil quenched, fine grained, tempered at 540°C | Tensile Strength (MPa) | 1082 |
Yield Strength (MPa) | 979 | ||
Elongation (%) | 17 | ||
Reduction in Area (%) | 51 | ||
25 | oil quenched, fine grained, tempered at 650°C | Tensile Strength (MPa) | 883 |
Yield Strength (MPa) | 793 | ||
Elongation (%) | 22 | ||
Reduction in Area (%) | 60 |